Why Do Molded Silicone Goods Keep Tearing? How To Select High‑Tear HTV Molding Silicone Rubber

Hits: 1645 img

Tearing, fracture and demolding damage are common pain‑points in compression‑molded silicone manufacturing. For items such as watch bands, ornaments, rubber bands and protective sleeves subjected to repeated stretching and bending, the raw HTV silicone compound must deliver high tear resistance, good elongation and favorable mold‑release performance. Conventional HTV rubber often yields defective parts with low yield rates. Therefore, proper material selection for high‑tear heat‑vulcanized molding silicone has become a key concern for silicone fabricators.

This article introduces a high‑tear HTV molding silicone series covering hardness from 25 to 70 Shore A with translucent appearance. It features high tensile property and excellent mold‑release behavior for smooth compression‑molding processing. The material has passed RoHS, REACH and FDA relevant tests to meet compliance requirements for consumer‑grade silicone exports.

Typical Performance Data

Note: Test specimens cured with 1% addition of 50% DBPH‑50 peroxide, 175 ℃, 15 MPa, 5 min curing, 2 mm test sheet. All figures are typical reference values only, not for formal acceptance specification. Final specifications shall be agreed between parties before order.

Model HTV‑313‑20 HTV‑313‑30 HTV‑313‑40 HTV‑313‑50 HTV‑313‑60 HTV‑313‑70
Appearance Translucent Translucent Translucent Translucent Translucent Translucent
Plasticity 140 160 200 220 240 280
Hardness (Shore A) 25 30 40 50 60 70
Density(g/cm³) 1.10 1.12 1.14 1.18 1.20 1.23
Tensile Strength(MPa) 7 8 8 8 8 7
Elongation at Break(%) 800 850 750 650 500 400
Tear Strength(kN/m) 14 20 30 30 22 22

Processing & Storage Guidelines

  1. Vulcanization: Recommended loading: 1% of 50% DBPH‑50 peroxide. Standard molding condition:175 ℃ ×5 min @15 MPa. Adjust temperature & dwell time according to part thickness and mold geometry.
  2. Packaging: 20 KG per carton.
  3. Shelf‑life: 18‑month shelf‑life from production date for unopened packages stored ≤50 ℃. Expired stock shall be fully re‑tested before production usage, only qualified batches can be adopted for manufacturing.

Main Applications

Compression‑molded protective sleeves, silicone wallets, smart‑watch bands, elastic rubber bands and decorative ornaments requiring repeated flexing and stretching.

Selection Tips

  1. Soft grades (20‑30 A) focus on high elongation; optimum tear performance falls within 30‑50 Shore A. Harder grades feature reduced elongation for low‑deformation structural components.
  2. For EU & US export, verify RoHS, REACH and FDA compliance documents for target‑market regulatory compliance.
  3. Perform trial molding before mass production to validate mold‑release behavior and end‑product tear performance.

FAQ

Q: Can high‑tear HTV silicone directly replace ordinary molding silicone rubber?
A: Direct replacement is feasible, but pilot trial is strongly recommended. Fine‑tune peroxide dosage and curing cycle to confirm demolding and mechanical performance.

Q: Can expired rubber compound still be used?
A: Direct usage is not allowed. Complete re‑testing including tensile, tear and hardness is mandatory; only qualified material can go into production.

Q: Is this high‑tear compound compatible with platinum cure system?
A: This series is designed for peroxide curing system, DBPH‑50 is the standard option. If platinum curing is required, dedicated platinum grades are suggested. Do not mix platinum catalyst directly into this compound.

Q: Thin molded parts tend to stick to mold, what can be done to improve mold release?
A: First check peroxide dosage and curing time. Internal mold release agent or mold coating is preferred. Excessive external spray release agent is not recommended, which may hinder printing, painting or bonding in later processes.

Q: Is there a big difference in shrinkage rate between high‑tear HTV and regular HTV at the same hardness?
A: Shrinkage values are close for the same hardness, yet minor differences exist. Mold dimension verification via trial molding is necessary after switching materials to avoid out‑of‑spec parts.

Q: Can cured parts from this series be printed, painted or bonded?
A: The cured substrate supports screen printing, spray painting and adhesive bonding. Final adhesion depends on ink and glue selection. Adhesion test in advance is required, plasma surface treatment may be needed for some inks.

Q: Can different hardness grades be blended to get intermediate hardness?
A: Blending is technically possible, but tear strength and elongation will not change linearly. Performance fluctuation may occur. For custom hardness, ready grades are preferred.